How to repair tension marks on precision piston rods

If the precision piston rod is pulled during operation and not treated in a timely manner, it can affect the use of the product in mild cases, and in severe cases, make the hydraulic cylinder unable to work. So how do we fix it? Local grinding and polishing methods are used to repair lighter pull marks; For heavier pull marks, welding repair and manual grinding are used to repair them.
Formation of pull marks: After disassembling the gas-liquid booster cylinder, it was found that a precision piston rod was severely pulled, with 6 pull marks arranged side by side. The main reason for the pulling injury is that after the dust ring becomes brittle and falls off in a block like manner, it not only loses its dust prevention effect, but also accumulates a lot of dust and impurities in the expansion joint, causing the piston rod to grind hard with impurities, resulting in pulling injury. The scars then scratch the rubber sealing components at the cylinder port, causing serious leakage of the hydraulic cylinder.
Repair requirements: The filler and base material should be combined stably and smoothly; The seasoning must be easy to use and easy to manually process; Manual processing should ensure that the diameter error of the precision piston rod is less than 0.06mm. After analysis, it was decided to use J422 welding rod as the filler. Because acidic welding rods are not sensitive to rust, oil stains, and moisture, and are not prone to generating hydrogenated pores; Good craftsmanship and easy operation; Beautiful welding seam formation; The material has moderate hardness and is easy to process by hand; Stable arc, large melting depth, and stable bonding with the base material.
Repair process:
1. Clean the area to be welded first, and then surround the pull marks with damp mud.
2. Select a welding rod with a diameter of 2.5mm, adjust the current of the welding machine to 120A, and use the straight line welding method to smoothly weld.
3. After all welding is completed, clean the mud and slag, and use a rough file to file along the circumference of the precision piston rod, leaving a machining allowance of 0.1-0.2mm.
4. A cylinder with an outer diameter of 185mm, an inner diameter of 125mm, and a length of 150mm is used as a model (the outer diameter of the piston rod is 125mm). It is sawn along the axis, with one being a rough model and the other being a precision model.
5. Apply a thin layer of red ink on the inner wall of the rough mold, and then rub the rough mold tightly against the area to be repaired along the axis several times. Then, use a fine file to remove the heavier red ink on the product. Repeat the filing process and leave a machining allowance of 0.04-0.07mm.
6. Then use a 320 mesh sand strip dipped in kerosene and fine mold to grind the product to the specified size.
7. Afterwards, dip the back of the sandcloth in kerosene for manual polishing. After measurement, the significant error is only 0.03mm.

主站蜘蛛池模板: 免费a级毛片在线观看 | 久久国产精品99久久久久久牛牛 | 久碰人澡人澡人澡人澡91 | 精品一区二区视频在线观看 | 一级毛片日韩a欧美 | 黄网站免费在线观看 | 欧美三级在线观看不卡视频 | 成人a大片高清在线观看 | 国产一区二区三区在线视频 | 精品国产三级a∨在线观看 精品国产三级a在线观看 | 日本三级2019 | 天天玩天天操 | 久996视频精品免费观看 | 欧美国产中文 | 日日操日日操 | 天天天天做夜夜夜夜 | 欧美日韩亚洲一区二区三区 | 青青久久国产成人免费网站 | 大乳护士好爽免费视频 | 日本一级网站 | 精品欧美一区二区三区免费观看 | 日韩美视频网站 | 91在线品视觉盛宴免费 | 亚洲欧美另类在线视频 | 午夜天堂在线 | 国产亚洲欧美一区 | 色香色香欲天天天影视综合网 | 一本一道波多野结衣一区二区 | 男女性高爱潮免费看 | 午夜在线观看完整高清免费 | 亚洲精品一二三区-久久 | www.久久.com| 国产精品99久久久久久宅男 | 老司机精品视频在线 | 国产一区二区影院 | 亚洲精品国产经典一区二区 | 91精品视频在线播放 | 99re6这里有精品热视频在线 | 天天综合在线观看 | 日本免费观看日本高清视频 | 亚洲欧美日韩综合在线播放 |